产品推荐
基本参数
厂商 | 美国 | 牌号 | KT-851 |
特性级别 | 阻燃级 | 用途级别 | 耐热级 |
类型 | 标准料 | 加工级别 | 挤出级 |
厂家 | 美国苏威 | 截面形状 | 粒子 |
执行标准 | 美标 | 材质 | PEEK |
每件重量 | 25kg |
KetaSpire? KT-851
聚醚醚酮
Solvay Specialty Polymers
产品说明:
KetaSpire? PEEK is produced to the highest industry standards and is characterized by a distinct combination of properties, which include excellent chemical resistance to organics, acids and bases, best in class fatigue resistance, excellent wear resistance, ease of melt processing and high purity.
The pellets are supplied with a very light dusting (0.01%) of calcium stearate to aid with conveying through single screw extruder-based processing equipment.
Natural: KetaSpire? KT-851 NT
基本信息 | |
---|---|
黄卡编号 | |
添加剂 |
|
特性 |
|
用途 |
|
RoHS 合规性 |
|
外观 |
|
形式 |
|
加工方法 |
|
物理性能 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
比重 | 1.30 | g/cm3 | ASTM D792 |
熔流率(熔体流动速率)(400°C/2.16 kg) | 10 | g/10 min | ASTM D1238 |
收缩率 | ASTM D955 | ||
流动 | 1.1 到 1.3 | % | ASTM D955 |
横向流动 | 1.3 到 1.5 | % | ASTM D955 |
吸水率(24 hr) | 0.10 | % | ASTM D570 |
硬度 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
洛氏硬度(M 级) | 97 | ASTM D785 | |
肖氏硬度(邵氏 D, 1 秒) | 88 | ASTM D2240 |
机械性能 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
拉伸模量 | |||
--1 | 3600 | MPa | ASTM D638 |
-- | 3850 | MPa | ISO 527-2/1A/1 |
拉伸应力 | |||
屈服 | 95.0 | MPa | ISO 527-2/1A/50 |
-- | 96.0 | MPa | ASTM D638 |
伸长率 | |||
屈服2 | 5.2 | % | ASTM D638 |
屈服 | 4.8 | % | ISO 527-2/1A/50 |
断裂3 | 20 到 30 | % | ASTM D638 |
断裂 | 20 到 30 | % | ISO 527-2/1A/50 |
弯曲模量 | |||
-- | 3900 | MPa | ASTM D790 |
-- | 3620 | MPa | ISO 178 |
弯曲强度 | |||
-- | 152 | MPa | ASTM D790 |
-- | 112 | MPa | ISO 178 |
压缩强度 | 121 | MPa | ASTM D695 |
剪切强度 | 91.5 | MPa | ASTM D732 |
冲击性能 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
悬壁梁缺口冲击强度 | |||
-- | 69 | J/m | ASTM D256 |
-- | 7.5 | kJ/m2 | ISO 180 |
无缺口悬臂梁冲击 | 无断裂 | ASTM D4812, ISO 180 |
热性能 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
载荷下热变形温度4(1.8 MPa, 退火, 3.20 mm) | 157 | °C | ASTM D648 |
玻璃转化温度 | 150 | °C | ASTM D3418 |
熔融峰值温度 | 340 | °C | ASTM D3418 |
线形热膨胀系数 - 流动(-50 到 50°C) | 4.3E-5 | cm/cm/°C | ASTM E831 |
比热 | DSC | ||
50°C | 1350 | J/kg/°C | DSC |
200°C | 1950 | J/kg/°C | DSC |
导热系数 | 0.24 | W/m/K | ASTM E831 |
电气性能 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
表面电阻率 | 1.9E 17 | ohms | ASTM D257 |
体积电阻率 | 2.5E 17 | ohms·cm | ASTM D257 |
介电强度(0.0500 mm, 非晶膜) | 200 | kV/mm | ASTM D149 |
充模分析 | 额定值 | 单位制 | 测试方法 |
---|---|---|---|
熔体粘度(400°C, 1000 sec^-1) | 380 | Pa·s | ASTM D3835 |
补充信息 |
---|
Standard Packaging and Labeling KetaSpire resins are packaged in polyethylene buckets or cardboard boxes depending upon the order size. Individual packages will be plainly marked with the product, color, lot number, and net weight. |
注射 | 额定值 | 单位制 | |
---|---|---|---|
干燥温度 | 150 | °C | |
干燥时间 | 4.0 | hr | |
料筒后部温度 | 355 | °C | |
料筒中部温度 | 365 | °C | |
料筒前部温度 | 370 | °C | |
射嘴温度 | 375 | °C | |
模具温度 | 175 到 205 | °C | |
注射速度 | 快速 | ||
螺杆压缩比 | 2.5:1.0 到 3.5:1.0 |
注射说明 |
---|
Drying KetaSpire resins must be dried completely prior to melt processing. Incomplete drying will result in defects in the formed part ranging from surface streaks to severe bubbling. Pellets can be dried on trays in a circulating air oven or in desiccating hopper dryer. Drying conditions recommended are 4 hours at 150°C (300°F) . Injection Molding KetaSpire resins can be readily injection molded in most screw injection machines. A general purpose screw with a compression ratio in the range of 2.5 - 3.5 : 1 is recommended, as is minimum back pressure. Injection speeds should be as fast as possible, consistent with part appearance requirements. Mold temperatures in the range of 175°C to 205°C (350°F to 400°F) are suggested. Recommended starting point barrel temperatures are shown in the following table. |
备注 | |
---|---|
1 . | 1.0 mm/min |
2 . | 50 mm/min |
3 . | 50 mm/min |
4 . | 200°C,2小时 |
上海汇堡材料科技有限公司
联系人:
唐经理
服务热线:
ꌙ풂줒혁줗륖풂혁
ꌙ풂줒혁줗륖풂혁
公司地址:
上海市金山工业区夏宁路666弄58-59号
-
食品级 POM N2320-0038 德国巴斯夫 高抗冲;耐热 Ultraform¥23.5元
-
Ultraform POM N 2320 U03 德国巴斯夫 抗紫外线性能良好¥24.5元
-
抗紫外线聚甲醛 N 2320 U035 德国巴斯夫 POM Ultraform®¥24.5元
-
PA66 Zytel 美国杜邦 BM70G20HSLX BK537 尼龙66 玻璃纤维增强20%¥46元
-
矿物填料30% FR70M30V0BK010 PA66 Zytel 美国杜邦 尼龙66¥55元
-
尼龙66 Zytel 70G35HSL 美国杜邦 PA66 原厂原包 一对一票 加纤35%¥54元
-
加纤43%尼龙66 70G43HSLA BK099 美国杜邦 PA66 Zytel¥55元
-
尼龙66 美国杜邦 70G35HSLRA4 PA66 Zytel 纤维增强35%¥55元
PEEK聚醚醚酮 KT-851 美国苏威 耐化学 电线护套 电气 石油 汽车应用相关产品
- PEEK原料 威格斯 450G 耐高温 注塑PEEK 挤出PEEK 国产PEEK
- PEEK碳纤 威格斯 450CA30 30%碳纤增强 耐磨 耐高温336 PEEK阻燃
- PEEK生产商 威格斯 150GL30 30%GF 耐磨 耐高温 PEEK材料
- PEEK 本色 咖啡色 玻纤增强 耐磨 高强度 耐化学 耐温328 防火V0
- 本色 黑色 PEEK板 耐高温 PEEK棒 防静电PEEK板材 褐色PEEK板
- 本色peek板 按规格需求定制加工 peek板材 进口原料防静电耐
- 供应peek板 按规格切割 加纤PEEK板/防静电peek 黑色本色褐色齐全
- 热销 良好的流动性 耐化学 PEEK树脂 450G 挤出级板材棒材专案料
- PEEK炭黑导电级东莞宇硕/YSFKB-A300 导电PEEK耐高温材料厂家直销
- PEEK/英国威格斯/450g 高刚性peek高强度 peek塑胶原料
- VICTREX® PEEK 450CA30
- 直销耐磨PEEK 沙伯基础(原GE) LF100-12耐高温 聚醚醚酮 填充PEEK
- 30%碳纤增强PEEK 英国威格斯 450CA30耐磨 高强度 高刚性peek塑料
- 优惠出售高强度PEEK 英国威格斯 450GL30增强30% 阻燃耐高温peek
- 厂家直销 PEEK本色加纤耐高温330度耐磨级耐化学PEEK耐高低温塑料
- 厂家直销 PEEK本色加纤耐高温330度耐磨级耐化学级PEEK耐高低温塑料
- 厂家直销 PEEK本色加纤耐高温330度耐磨级耐化学性PEEK耐高低温塑料
- 厂家直供 PEEK本色加纤耐高温330度耐磨级耐化学PEEK耐高低温塑料原料材料
猜你在找
- 英国威格斯 聚醚醚酮粉 450P粉 500目 共混改性用PEEK
- 聚醚醚酮PEEK 基础创新塑料 美国 L1000 注塑级 医用级 电子电器部件 现货
- PEEK 基础创新塑料 美国 LL004C 注塑级 PEEK食品接触应用粉料PEEK专注医疗保健PEEK高流动耐化学粉料
- 聚醚醚酮PEEK 基础创新塑料 美国LF1006注塑级
- 宏裕销售PEEK 基础创新塑料 美国 LFL-4031 BK 注塑级 PEEK专注医疗保健 peek
- 聚醚醚酮PEEK 基础创新塑料 美国LF-1004注塑级
- 聚醚醚酮PEEK 基础创新塑料 美国LCL-4036EM注塑级 医用级 电子电器部件 现货
- PEEK 基础创新塑料美国 L1000 粉 注塑级 注塑级 粉料供应
- PEEK 基础创新塑料美国 LC005 BK 注塑级
- 聚醚醚酮PEEK 基础创新塑料 美国LFL-4036注塑级
- 宏裕销售PEEK 基础创新塑料 美国PDX-L-92134 NAT 注塑级 PEEK专注医疗保健 peek
- 聚醚醚酮PEEK 基础创新塑料 美国 LF-1002 注塑级耐化学品腐蚀阻燃耐剥离性耐磨性
免责声明:以上展示的PEEK聚醚醚酮 KT-851 美国苏威 耐化学 电线护套 电气 石油 汽车应用信息由上海汇堡材料科技有限公司自行提供,内容的真实性、准确性和合法性由发布企业负责,